Skip to main content

Table 1 Weight loss of Mega-PK- and Mega-L-treated cotton fabrics

From: Effects of biopolishing on the quality of cotton fabrics using acid and neutral cellulases

Sample no.

Concentration (%)

Temperature (°C)

Time (min)

Weight loss (%)

Mega PK

Mega L

1

0.5

45

40

0.25

0.2

2

0.5

55

40

0.27

0.24

3

0.5

65

40

0.29

0.27

4

0.5

45

50

0.26

0.31

5

0.5

55

50

0.31

0.35

6

0.5

65

50

0.29

0.38

7

0.5

45

60

0.33

0.42

8

0.5

55

60

0.35

0.45

9

0.5

65

60

0.39

0.49

10

1

45

40

0.62

0.61

11

1

55

40

0.65

0.66

12

1

65

40

0.69

0.71

13

1

45

50

0.72

0.74

14

1

55

50

0.70

0.79

15

1

65

50

0.76

0.82

16

1

45

60

0.82

0.84

17

1

55

60

0.86

0.86

18

1

65

60

0.89

0.88

19

1.5

45

40

0.98

0.95

20

1.5

55

40

1.05

0.97

21

1.5

65

40

1.12

0.99

22

1.5

45

50

1.17

1.02

23

1.5

55

50

1.21

1.06

24

1.5

65

50

1.26

1.09

25

1.5

45

60

1.32

1.13

26

1.5

55

60

1.36

1.17

27

1.5

65

60

1.42

1.22